13.12 Soldering
A jumper wire in a breadboard holds on a quiet bench, but on any vibrating machine it works loose. A solder joint is a metallic bond: molten solder wets both metal surfaces, and when it sets the two parts form one conductor. Here we cover hand soldering of wire joints and through-hole technology (THT) components on perfboards. As mechanical engineers, we build one-off and few-off prototypes, i.e., proofs of concept. Turning a working prototype into a production board with surface-mount (SMD) parts is a job for electrical engineers, so SMD soldering is left out here.
The photos use an RC car build as a running example. Every joint shown was made by a beginner, and none would win a beauty contest. Every one held a hard tug, none is cold, and none bridges to its neighbour.
The Guide
Tools and materials
| Item | Use |
|---|---|
| soldering iron with temperature control | set to 350 °C at most |
| a powerful iron with a large chisel tip | heavy connectors (e.g. XT60) and thick AWG 16 leads |
| silicone-insulated wire | flexible, heat-resistant hook-up and power leads |
| solder: Weller WSW SAC M1, 0.8 mm, resin core | Sn 96.5 %, Ag 3.0 %, Cu 0.5 %, 3.5 % flux, 217 to 221 °C |
| soldering greasesv. lödfett (Felder, DIN EN ISO 9454-1: 3214) | thin coat on every surface before soldering |
| tip cleaner (RS PRO lead-free tip tinner) and moist sponge | restores and wipes an oxidised tip |
| cross-locking tweezerssv. låspincett | holds small parts on the board while flipping and soldering |
| heat-shrink tubingsv. krympslang or insulating tapesv. isoleringstejp | over every joint on a wire |
| isopropyl alcohol and a small brush | removes flux residue after soldering |
| desoldering braid or solder pump | removes solder |
| multimeter | continuity check for bridges |
Our solder is 0.8 mm lead-free Weller WSW SAC M1 (Figure 13.12.2), a tin-silver-copper alloy (SAC305: Sn 96.5 %, Ag 3.0 %, Cu 0.5 %, melting at 217 to 221 °C). A 3.5 % resin flux core runs down its centre (Figure 13.12.2 (b)). The 3 % silver content matters for hand soldering: compared with silver-free tin-copper alloys, it lowers the melting point and improves flow and wetting, making lead-free joints much easier for beginners.
Alongside it on the bench is a 50 g tin of Felder soldering greasesv. lödfett (Figure 13.12.3), a firm amber paste classified under DIN EN ISO 9454-1 as type 3214.
Type 3214 is an inorganic flux whose active salt is zinc chloride in a fatty carrier. It strips copper oxide fast, making thick wires and XT60 cups far easier to tin than with the mild flux core alone. Because zinc chloride is corrosive and draws moisture, unburned residue slowly attacks copper and can leak current between close pins; production electronics therefore use non-corrosive rosin or no-clean flux (ISO 9454-1 class 1). For prototypes we use this grease sparingly and scrub boards clean with isopropyl alcohol afterwards.
We use silicone-insulated wire only (Figure 13.12.4). Unlike PVC, silicone resists soldering heat without melting or shrinking back from the joint, so the bare length stays as stripped. It strips cleanly and stays flexible, letting the wire bend along its length under vibration instead of fatiguing the joint.
The tip is at 350 °C and the joint stays hot for several seconds after the iron leaves it. Put the iron back in its stand every time it leaves your hand, and hold wires with pliers or a clamp, never with your fingers. The smoke is burning flux, which irritates the airways and, breathed in over time, can cause asthma. Solder by an open window or a fume extractor, keep your face out of the plume, and wear safety glasses: zinc-chloride grease causes serious eye damage on contact (Figure 13.12.3 (a)). Keep it off your skin and wash your hands afterwards.
Step 1: Heat and tin the tip
Set the iron to 350 °C at most. Hotter does not solder faster: the tip oxidises sooner, and the flux burns off before it has done its work. When the iron is hot, melt a little solder on the tip. A good tip takes the solder at once and turns bright and shiny.
A tip that stays matt and lets the solder roll off (Figure 13.12.5) is oxidised. We restore it with the bench tip tinner (Figure 13.12.6), a solid lead-free paste of solder powder and ammonium phosphate that strips oxide and re-tins the iron plating in one step.
Press the hot tip (350 °C) into the paste and turn it until the paste melts over the end. Wipe it on a moist sponge and touch fresh solder wire to it. The sequence in Figure 13.12.7 shows a tip stored for several months returning to a bright, wetted end. Stubborn oxide may take two or three rounds.
Step 2: Soldering grease on both surfaces
Slide the heat-shrink tube onto the wire first, well away from the joint. It cannot go on once both ends are soldered.
Strip the wire and twist the strands tightly so no strand sticks out. A stray strand is the most common short circuit on a beginner’s board, bending unseen onto the next pin.
Use the soldering grease sparingly: dip the twisted end lightly into the grease (Figure 13.12.8 (a)) for a thin sheen, and dab a thin film onto any pad or terminal with a toothpick or scrap wire. Never dip the hot iron tip into the tin; zinc chloride corrodes the tip plating and charred grease spoils the tin. Without flux, molten solder beads up and rolls off the copper.
Step 3: Tin each part separately
Melt solder from the wire onto the tip and touch the greased surface (Figure 13.12.8 (b)). The grease sizzles, smokes, and strips oxide from both the strands and the solder drop, so solder wicks straight into the wire even if the drop on the tip has gone “dry”. Do the same on the second surface (Figure 13.12.11 (a)). Coating each part first is called tinning.
Tin the full stripped length of a wire so the strands bind into one solid lead. A thick wire takes more solder and more heat: drench it until solder soaks through to the middle strands (Thick wires and the XT60).
Trim the tinned end with side cutters so about 1 to 2 mm of bare wire extends past the insulation. Longer bare wire flexes and breaks strand by strand, or bridges onto a neighbouring pad. Two adjacent wires with 5 mm bare need only shift slightly to short together; a bare end must be too short to reach any pad or wire but its own (Figure 13.12.9 and Figure 13.12.10).
The smoke signals active flux. On the tip alone, flux burns off within seconds, leaving a dry drop that will not wet bare copper. Grease on the wire supplies fresh flux at contact; without grease, wipe a dry drop off the tip and melt a fresh one.
The video shows the difference at close range: without flux, solder beads on top of the strands under a wrinkled skin; with flux paste, the skin vanishes and solder soaks between the strands.
Step 4: Join the parts
Hold the two tinned parts still with pliers, a clamp, or a bent wire (Figure 13.12.11 (a)). Touch the joint with wet solder on the tip so both coatings melt together (Figure 13.12.11 (b)). Feed a little wire solder if needed, lift the iron, and hold steady until the joint sets.
Always heat through wet solder on the tip. A dry tip contacts the part at a point and heats slowly. Molten solder widens the contact area so the joint melts in a second or two (Why wet solder carries the heat).
Step 5: Tug and check
Once the joint cools, pull the wire firmly. A good joint holds; a cold joint, where solder never wetted one surface, slips or turns. Redo it with fresh soldering grease.
On a board, inspect neighbouring pins under good light for bridges, stray strands, and bare wire over 2 mm. Check continuity with a multimeter between adjacent pads that must stay separate, and remove any bridge with braid (Desoldering).
Scrub leftover grease off the perfboard and between close pins with isopropyl alcohol and a small brush before powering up or insulating.
Step 6: Insulate
Pick a sleeve that slips snugly over the joint (Figure 13.12.12 (a)), slide it into place, and shrink it with a hot-air gun or the shank of the iron, never the tip (Figure 13.12.12 (b) and Figure 13.12.12 (c)). For a Y-splice, where one wire splits into two, see Figure 13.12.13. Insulating tape also works; our first build used tape on every joint (Figure 13.12.19) and all of them held.
Step 7: Finish
Melt a fresh protective layer of solder onto the tip before switching the iron off, and leave it there (Figure 13.12.14). The solder seals the iron plating from air until the next session. Never leave a hot tip bare for long: an untinned tip oxidises within minutes.
Thick wires and the XT60
Thick AWG 16 wire and XT60 contacts hold a lot of copper, which pulls heat away from the tip rapidly. Use the large iron with a wide chisel tip; a small iron cools below the melting point on contact and never catches up.
Load the tip with a generous drop of solder for a wide thermal contact. Drench the wire first (Step 3), fill the contact cup with molten solder, push the tinned wire in, and hold still until it sets. Lift the iron as soon as the joint flows: prolonged heat softens the XT60 plastic housing and shifts the contact out of alignment. If it refuses to flow, let it cool, add soldering grease, and retry with more solder on the tip.
Parts that do not tolerate heat
Every component has a thermal limit. Overheating the main switch softens its plastic body and shifts the spring contacts until the switch jams. MOSFETs and chips typically tolerate soldering heat at their pins for about 10 s. Check the datasheet for the exact limit: for the IRL540 MOSFET (Figure 13.12.15), the maximum is 300 °C for at most 10 s, measured 1.6 mm from the case.
The rule is the same for all of them: be quick but effective.
Prepare everything first (flux paste on, both parts tinned, wet solder on the tip), so that the final joint needs only a second or two of heat. A joint that will not flow within a few seconds needs more flux or more solder on the tip, not a longer wait. Let a part cool before the next attempt.
Our joints
The photos in this section come from a student-built RC car and show working beginner joints made with the method above.
The power leads come first. The XT60 connector and the main switch carry the full motor current, so their joints get thick wire, the large iron, and plenty of solder (Figure 13.12.16, Figure 13.12.17, and Thick wires and the XT60). On the connector, solder fills the cup holding the wire.
The motor has two tabs at its rear end (Figure 13.12.18). Each wire is hooked through its tab and soldered.
The logic wires of the motor driver are soldered to its header pins from the underside (BTS7960, Step 1), alongside the 10 kΩ pull-down resistor on EN (Figure 13.12.20). With pins 2.54 mm apart, the Step 5 bridge check matters.
The screw terminals of the motor driver (Figure 13.12.21) take the wire without solder. Solder under a screw creeps slowly under the pressure, the clamp loosens, and a loose terminal at motor current gets hot. Twist the strands, push them in, and tighten.
The ESP32 perfboard
A perfboard is a plate with a hole every 2.54 mm and a copper ring around each hole, on which we build a circuit by hand. We never solder the ESP32 directly to the perfboard (Figure 13.12.22 (a)), because a damaged board would then be nearly impossible to remove. Instead, we use two strips of 2.54 mm female header sockets (Figure 13.12.22 (b)) so the DevKit plugs in and can be swapped at any time (Figure 13.12.1).
Plug the header strip onto the ESP32 to find the exact row length (Figure 13.12.22 (c)), then cut it with side cutters straight through the unwanted pin beside the last slot. Keep both cut headers plugged onto the ESP32 when you push them into the perfboard (Figure 13.12.23 (a)): the DevKit holds both rows parallel and square at the exact spacing. Flip the assembly over (Figure 13.12.23 (b)) and solder the header pins to their copper rings from the underside.
A through-hole joint follows the same method: a thin dab of soldering grease on the ring and pin, the wet tip against both at once, and a little solder from the wire. Without flux, dry solder clumps around the unwetted pin and bridges across to neighbouring holes (Figure 13.12.24 (a)). Adding a small dab of flux and reheating pulls the solder off the neighbour into a smooth cone around the pin (Figure 13.12.24 (b)). Solder both end pins of each header first and check that it lies straight and flat before soldering the rest, then solder the wires to the same pins (Figure 13.12.26).
Small parts such as a three-pin header fall out as soon as we flip the perfboard over. Cross-locking tweezerssv. låspincett clamp the part flat against the board so we can turn it over and solder with both hands free (Figure 13.12.25). Leave the clamp on while soldering the first pin; once that joint sets, remove the tweezers, check that the part is straight, and solder the remaining pins.
How It Works
Why flux
Solder bonds only to clean metal, where solder atoms meet copper atoms directly. In air, copper wire, pins, and molten solder all carry an invisible oxide skin. That barrier makes molten solder bead up like water on a greasy plate, and causes the wrinkled skin on unfluxed solder.
Flux is passive at room temperature, then activates near soldering temperature to dissolve oxide and shield the clean metal from air. Because it burns off as smoke within seconds, a drop left on the tip or a joint reheated repeatedly runs out of flux.
Androkavo’s video tracks this with an on-screen flux gauge. Flux-core wire brings enough flux for a joint and one or two reheats; after about three reheats the joint turns dull and lumpy until fresh paste restores a smooth cone (Figure 13.12.24).
Unburned flux leaves residue around the joint. Rosin from the solder core is benign under tape, whereas zinc-chloride residue from our soldering grease draws moisture and corrodes copper, so wipe wire joints and scrub boards with isopropyl alcohol and a brush.
Why wet solder carries the heat
Two solid metals touch only at microscopic high points, separated by air that conducts heat poorly. Molten solder fills the gap and conducts heat more than a thousand times better than air, expanding the contact to the full wetted area so the joint melts in a second or two.
Never heat a joint with a dry tip: molten solder is the thermal bridge between iron and copper.
On a heavy joint such as an XT60, the iron must also deliver heat as fast as the copper drains it. A large iron with a heavy chisel tip stores more heat and keeps its temperature above the melting point on contact.
Temperature and the tip
Lead-free SAC305 melts at 221 °C, about 40 °C above tin-lead solder. Setting the iron to 350 °C leaves a 130 °C margin for thick AWG 16 leads without accelerating tip oxidation or burning off flux prematurely.
The tip is iron-plated copper. Once its surface oxidises into a matt layer (Figure 13.12.5), solder no longer wets it and heat transfer stops until tip tinner strips the oxide (Figure 13.12.7). Leaving fresh solder on the tip at Step 7 seals the iron from air between sessions. Good lead-free joints look slightly less glossy than tin-lead ones, whereas a cold joint is grainy, sharp-edged, and fails the tug test.
Desoldering
Before replacing a part or clearing a stubborn bridge, remove the old solder. Lay copper desoldering braid across the joint and press the iron on top so molten solder wicks into the braid (a dab of flux helps). A solder pump works by cocking the plunger, melting the joint, and triggering the nozzle beside it. Neither clears every trace, so heat a stuck pin and ease it loose.
For a two-pin part, adding more solder to bridge both pins lets the iron melt both joints together. Excessive heat or pulling before the solder melts lifts the copper pad off the board.
Exercises
1. Read the joint. After a joint, the solder beads on the wire with a wrinkled skin and bright copper strands underneath. What was missing, and how do you redo the joint?
2. Nothing melts. The iron is at 350 °C, the solder on the tip melts, but a thick motor lead stays cold for half a minute and the solder from the wire will not stick to it. Give two causes and the fix for each.
3. Three tries. You have heated the same joint four times and it now looks dull and grainy. Why does a fifth heating with the iron alone not help, and what does?
4. Tin a lead. Strip 8 mm of an AWG 16 wire and tin it with the method of Step 3. Cut the tinned end through with side cutters and look at the cut: has the solder reached the strands in the middle?